Notes On Soft Soldering - AH00.19-P-1000-07A

Model All (4xWD, CAR, Heavy transporter, Light transporter, smart) 

General 

Soft soldering is a process for creating an inseparable connection between two or more metal parts using additional metals (e.g. soldering tin). The solder melting temperature is lower than the melting temperature of the metals to be joined and is less than 450°C.

The connection is created by wetting the joint locations with hot liquid solder, without melting the parts to be joined.

The connection procedure is assisted by using a flux, which releases surface oxides onto the parts to be joined, eliminating and preventing surface films (e.g. greases).

Soft soldering materials 

The soldering alloy determines its melting point and thus the working temperature during the soft soldering process. Additives modify the properties. Improving silver components, e.g. the surfaces and joining properties. Observe use of unleaded solder.

Soft solders are identified according to DIN EN 61190-1-3 or DIN EN 294453/ISO 9453.

Example: ELSOLD soft solder FLOWTIN TC07 Sn99, 7Cu0.7 The alloy consists of 99.7 % tin (Sn) and 0.7 % copper (Cu)

The melting range is 227°C.

Fast solders with a melting point range from approx. 180°C to 227°C should be used in the electrics/electronics area of vehicles. These solders are available in the form of wires. They have flux from resins dissolved in alcohol (e.g. colophonium) in their hollow center.

Soldering equipment 

Soldering equipment with soldering tips that can reach a temperature of 250°C to 300°C are suitable for repairs specified by Daimler. The aim is to use temperature-regulated automatic devices (e.g. soldering stations).

Preparation, general 

Preconditions for soldering 

Soldering points must be clean, free of grease and oxides.