BMW/Mini Bonding Instructions Rep-Alg-Rag1141-4105402 - V.11
Required Special Tools :
- 2 357 309
Attention!
CONFORM WITH SAFETY REGULATIONS! .
- Brief overview of surface preparation
1.1 Structure
| Material (surface condition) Type of repair |
Preparation |
|---|---|
| Aluminum (used part) Repairs on front end/rear end Example: Replacement of engine mount or front wheel arch |
|
| Aluminum (new part) Repairs on front end/rear end Example: Replacement of engine mount or front wheel arch |
|
| Carbon Fiber Reinforced Plastic (new part) Bonding new parts on the body using K1 adhesive in conjunction with blind rivets Example: Replacement of rear wheel arch |
|
| Carbon Fiber Reinforced Plastic (used part) Bonding new parts on the body using K1 adhesive Example: Replacement of B-pillar |
|
| Sheet steel (used part and new part) Partial replacement of components Example: Replacement of B-pillar or rear wheel arch |
|
1.2 Outer skin (without roof outer skin made of aluminum/CFRP)
| Material (surface condition) Type of repair |
Preparation |
|---|---|
| Sheet steel (used part) Adhesion for outer skin component Example: Replacement of rear quarter panel or tail panel |
|
| Sheet steel (new part) Adhesion for outer skin component Example: Replacement of rear quarter panel or tail panel |
|
1.3 Roof outer skin made of aluminum/CFRP
| Material (surface condition) Type of repair |
Preparation |
|---|---|
| Aluminum (new part) Bonding a roof outer skin made of aluminum |
|
| Sheet steel (primer undamaged) Bonding a roof outer skin made of aluminum |
|
| Sheet steel (primer damaged) Adhesion for roof outer skin |
|
| Carbon Fiber Reinforced Plastic (used part) Adhesion for roof outer skin |
|
| Carbon Fiber Reinforced Plastic (new part) Adhesion for roof outer skin |
|
2.1 The following basic conditions apply to all bonding:
- The working temperature of glue cartridge must be more than 18°C.
- Object temperature, vehicle and new parts, at least 15°C.
- Refer to the vehicle-specific REP for the position and thickness of the adhesive bead.
- After applying the adhesive, check whether an adhesive component has emerged at the back of the glue cartridge. If yes, break off the bonding procedure. Clean new part. Use new glue cartridge.
- Join components and secure in position.
- Remove excess adhesive. Do not use solvent cleaning agents.
2.2 Surface preparation (structural):
2.2.1 Flame-coating (aluminum):
- Clean bonding surfaces with cleaning agent R1.
- Remove oxide layers or paint from bonding surfaces using a stainless steel wire brush or sandpaper with 120 graining.
- Clean bonding surfaces with cleaning agent R1.
Allow cleaned surfaces to dry for approx. 5 min.
Bonding surfaces must be completely dry.
2.2.2 Surface preparation (Carbon Fiber Reinforced Plastic new part):
This surface preparation applies to new CFRP parts.
Remove coarse dirt from the bonding surfaces using solvent cleaner R2.
Clean bonding surfaces with cleaning agent R1.
Bonding surfaces with sanding using | non-woven abrasive.
Clean bonding surfaces with cleaning agent R1.
Let cleaned bonding surfaces dry for at least 2 min.
Bonding surfaces must be completely dry.
Activate bonding surfaces with Betawipe 4800.
Let activated bonding surfaces dry for at least 2 min.
Bonding surfaces must be completely dry.
2.2.3 Surface preparation (Carbon Fiber Reinforced Plastic used part):
This surface preparation applies to the top area of the B-pillar.
Attention!
Carbon Fiber Reinforced Plastic component not damaged!
Components must be replaced if showing signs of damage.
Remove coarse dirt from the bonding surfaces using solvent cleaner R2.
Clean bonding surfaces with cleaning agent R1.
Grind off adhesive residue to a thickness of approx. 0.5 mm.
Clean bonding surfaces with cleaning agent R1.
Let cleaned bonding surfaces dry for at least 2 min.
Bonding surfaces must be completely dry.
2.3 Surface preparation (outer skin (without roof outer skin)):
The procedure is described here.
2.4 Surface preparation (roof outer skin):
2.4.1 Surface preparation of roof frame and convertible top bow from sheet steel:
Cut back adhesive remnants (1) with scraper 2 357 309 to a minimum of 0.5 mm.
Primed surface must not be damaged.
Smaller damage to 5 mm or scratch marks can be ignored.
In the event of larger damage to primer (greater than 5 mm), proceed as follows:
Clean damaged area with cleaning agent R1.
Apply K5 adhesive to the bare areas using a spatula or (fine) brush. Apply a uniformly thin layer (max. 0.5 mm). After a curing period of 24 hours, the roof outer skin can be bonded.
The adhesive flange area must not be painted over when the roof frame is being repaired or renewed.
2.4.2 Surface preparation of Carbon Fiber Reinforced Plastic (used part):
Remove coarse dirt from the bonding surfaces using solvent cleaner R2.
Clean bonding surfaces with cleaning agent R1.
Cut back adhesive bead with scraper 2 357 309 to a minimum of 0.5 mm.
Clean bonding surfaces with cleaning agent R1.
Let cleaned bonding surfaces dry for at least 2 min.
Bonding surfaces must be completely dry.
2.4.3 Surface preparation of Carbon Fiber Reinforced Plastic (new part):
Prepare the surface as described under point 2.2.2.