51 31 ... Instructions on gluing windscreen: Notes
IMPORTANT:
The following topics were included or amended in March 2005:
Storage temperature of all adhesive products of 5°C to 25°C must be observed.
Special instructions for hot processing must be observed:
- Temperature of cartridge oven must be checked every morning with DIS or GT1
- Temperature of cartridge < 80°C results in the formation of bubbles/blisters (gluing/cementing not permitted)
- Insufficient heating (< 1 hour) results in the formation of bubbles/blisters (gluing/cementing not permitted)
- Heating time or a cartridge max. 8 hours
- Mistake in mixing in event of an interruption in application >1 minute (gluing/cementing not permitted)
- A test bead of 50...70 mm must be rejected after an interruption in application
- Cartridge may only be heated up once; if the lower label is black, this adhesive may only still be used cold without accelerator while adhering to the best before date.